June Perry on wed 29 may 02
Here's one for cone 8-10 You might try subbing Nepheline Syenite for the
Potspar, which may bring it down two cones. You can try subbing Alberta Slip
for the Albany if you don't have Albany.
#727 METALLIC CHARCOAL OR OIL SPOT C 8-10
ALBANY SLIP 73
BURNT SIENNA 9
POTASH FELDSPAR 9
RED IRON OXIIDE 5
HARDWOOD ASH 4
TOTAL 100
RRegards,
June Perry
| |
|