cone 6 ox oil spot

updated tue 4 jun 02

 

June Perry on thu 30 may 02


Here's one for cone 8-10 You might try subbing Nepheline Syenite for the
Potspar, which may bring it down two cones. You can try subbing Alberta Slip
for the Albany. I would even, for experiment sake, try subbing some of the
Albany or Alberta with some Redart or other earthenware clay.

#727 METALLIC CHARCOAL OR OIL SPOT C 8-10

ALBANY SLIP 73
BURNT SIENNA 9
POTASH FELDSPAR 9
RED IRON OXIIDE 5
HARDWOOD ASH 4
TOTAL 100

Regards,
June Perry

Tony Ferguson on mon 3 jun 02


To the Texans,

I have a friend in Dallas and she is looking to take some pottery classes.
So, anyone who knows a good place please let me know and I will forward her
your information.

Thank you.

Tony Ferguson
Stoneware, Porcelain, Raku
www.aquariusartgallery.com
218-727-6339
315 N. Lake Ave
Apt 312
Duluth, MN 55806



----- Original Message -----
From: "June Perry"
To:
Sent: Thursday, May 30, 2002 6:21 AM
Subject: Cone 6 OX oil spot


> Here's one for cone 8-10 You might try subbing Nepheline Syenite for the
> Potspar, which may bring it down two cones. You can try subbing Alberta
Slip
> for the Albany. I would even, for experiment sake, try subbing some of
the
> Albany or Alberta with some Redart or other earthenware clay.
>
> #727 METALLIC CHARCOAL OR OIL SPOT C 8-10
>
> ALBANY SLIP 73
> BURNT SIENNA 9
> POTASH FELDSPAR 9
> RED IRON OXIIDE 5
> HARDWOOD ASH 4
> TOTAL 100
>
> Regards,
> June Perry
>
>
____________________________________________________________________________
__
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.
>