search  current discussion  categories  glazes - cone 4-7 

glaze test for kleinsfield gold, cone 6-7 ox.

updated fri 14 jun 02

 

Alisa Liskin Clausen on thu 13 jun 02


Glaze test for Kleinsfield Gold, cone 6-7, ox.

Glaze tested on white midrange stoneware fired in electric oxidation to =
1220c.

Source: Clayart
Credited to: Jeff Dietrich

Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1100c (330f - 2012f)=20
100c p/h to 1220c (212f - 2228f)
cool down max. per hour to 900c (1652f)
hold for one hour at 900c
shut off kiln

Recipe:
4.49 Magnesium Carbonate
20.23 Whiting
5.62 Wollastonite
56.18 Neph. Sye.
13.48 Ceder Heights Redart Clay

Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in precent =
to the 100 gram test batch.

Substitutions:Oldenwalder Clay for Redart

Results:
Gloss mustard gold glaze with slightly green cast, transparent. Runny =
but did not drip off tile. Crazed on my claybody.


Regards from Alisa in Denmark