Tony Ferguson on wed 26 jun 02
Maolica Glaze
Bisque to 03 FIRE to O5 (you can play with this range about a cone)
White Glaze (used under Stain/Frit Blend)
55 Frit 3124
5 Ball Clay
5 EPK
12 Flint
8 SuperPax
8 Kona (Soda) Feldpar
4 Glaze Rite (Binder)
Colerants
Use Stains of your choice:
4 Parts Frit 3124
1 Part Stain
dilute to brushable consistency
(You could add GB for better brushability)
Best on red earthenware body--more grog = pitting
0 Wax Bottom of Piece no less then 1/6 inch up from bottom
1 Glaze Piece with White first.
2 Let it set up until you can handle it without smudging glaze
3 Paint on surface with frit/stain colorant mixture from own container
You can also color the white glaze base with a colorant
and have a variety of solid colors with which to glaze with.
Hope this helps.
Thank you.
Tony Ferguson
Stoneware, Porcelain, Raku
www.aquariusartgallery.com
218-727-6339
315 N. Lake Ave
Apt 312
Duluth, MN 55806
| |
|