Michele Williams on mon 22 jul 02
Edouard,
At what cone should this recipe fire best?
Michele Williams
>
> From Dr. Chris Hogg's program:
> Flint 20
> Kaolin 5
> Nepheline 60
> Whitimg 8
> Zinc oxide 7
>
> Now a statement from Richard Zakin's program:
>
> "If glazes in this category contain reasonably strong melters
> they will be vitreous. Their high silica content encourages
> durability and transparency. Their normal alumina content
> discourages glaze flow even if strong melters are present.
> This is an excellent category for tranparent glazes."
>
>
> Later,
>
>
> Edouard Bastarache
> Irreductible Quebecois
> Indomitable Quebeker
> Sorel-Tracy
> Quebec
> edouardb@sorel-tracy.qc.ca
> http://sorel-tracy.qc.ca/~edouardb/
> http://perso.wanadoo.fr/smart2000/index.htm
>
>
____________________________________________________________________________
__
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.
>
Ababi on tue 23 jul 02
6^ (matte) and higher
Ababi
---------- Original Message ----------
>Edouard,
>At what cone should this recipe fire best?
>Michele Williams
>>
>> From Dr. Chris Hogg's program:
>> Flint 20
>> Kaolin 5
>> Nepheline 60
>> Whitimg 8
>> Zinc oxide 7
>>
>> Now a statement from Richard Zakin's program:
>>
>> "If glazes in this category contain reasonably strong melters
>> they will be vitreous. Their high silica content encourages
>> durability and transparency. Their normal alumina content
>> discourages glaze flow even if strong melters are present.
>> This is an excellent category for tranparent glazes."
>>
>>
>> Later,
>>
>>
>> Edouard Bastarache
>> Irreductible Quebecois
>> Indomitable Quebeker
>> Sorel-Tracy
>> Quebec
>> edouardb@sorel-tracy.qc.ca
>> http://sorel-tracy.qc.ca/~edouardb/
>> http://perso.wanadoo.fr/smart2000/index.htm
>>
>>
>____________________________________________________________________________
>__
>> Send postings to clayart@lsv.ceramics.org
>>
>> You may look at the archives for the list or change your subscription
>> settings from http://www.ceramics.org/clayart/
>>
>> Moderator of the list is Mel Jacobson who may be reached at
>melpots@pclink.com.
>>
>______________________________________________________________________________
>Send postings to clayart@lsv.ceramics.org
>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/
>Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.
Edouard Bastarache on tue 23 jul 02
Tom Buck said it was a C/6 glaze.
Later,
Edouard Bastarache
Irreductible Quebecois
Indomitable Quebeker
Sorel-Tracy
Quebec
edouardb@sorel-tracy.qc.ca
http://sorel-tracy.qc.ca/~edouardb/
http://perso.wanadoo.fr/smart2000/index.htm
----- Original Message -----
From: Michele Williams
To:
Sent: Monday, July 22, 2002 8:40 PM
Subject: Firing Temp Q
> Edouard,
>
> At what cone should this recipe fire best?
>
> Michele Williams
>
> >
> > From Dr. Chris Hogg's program:
> > Flint 20
> > Kaolin 5
> > Nepheline 60
> > Whitimg 8
> > Zinc oxide 7
> >
> > Now a statement from Richard Zakin's program:
> >
> > "If glazes in this category contain reasonably strong melters
> > they will be vitreous. Their high silica content encourages
> > durability and transparency. Their normal alumina content
> > discourages glaze flow even if strong melters are present.
> > This is an excellent category for tranparent glazes."
> >
> >
> > Later,
> >
> >
> > Edouard Bastarache
> > Irreductible Quebecois
> > Indomitable Quebeker
> > Sorel-Tracy
> > Quebec
> > edouardb@sorel-tracy.qc.ca
> > http://sorel-tracy.qc.ca/~edouardb/
> > http://perso.wanadoo.fr/smart2000/index.htm
> >
> >
>
____________________________________________________________________________
> __
> > Send postings to clayart@lsv.ceramics.org
> >
> > You may look at the archives for the list or change your subscription
> > settings from http://www.ceramics.org/clayart/
> >
> > Moderator of the list is Mel Jacobson who may be reached at
> melpots@pclink.com.
> >
>
>
____________________________________________________________________________
__
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.
| |
|