Betsy Cox on sun 4 aug 02
Hi i' am looking for the recipe for Burgundy Matte Raku glaze . Can =
anyone help? Thanks
Betsy Cox
Michelle Lowe on sun 4 aug 02
At 12:28 PM 8/4/2002 -0400, you wrote:
>Hi i' am looking for the recipe for Burgundy Matte Raku glaze . Can anyone help? Thanks
Try this one
Very dry Burgundy Red (NICE glaze)
>
>Gerstley Borate 50
>Neph Sy 20
>Talc 30
>Copper carb 3
-----------
Michelle Lowe potter in the Phoenix desert
http://www.desertdragonpottery.com
Mishy@desertdragonpottery.com
mishlowe@amug.org
\|/ |
-O- | |
/|\ | | |
|_|_|
____ |
\ /-----|-----
( )
<__>
Ababi on sun 4 aug 02
From Deg's list
Glaze name: Matt burgundy red
Color: red
Firing: Raku
Date: 05/13/98
Recipe: Percent Batch
Gerstley borate 48.5 50.00
Nepheline syenite 19.4 20.00
Talc 29.1 30.00
Copper carbonate 2.9 3.00
Totals: 100.0 % 103.00 g
Comments:
Reduce heavily. May need to be fired to slightly lower temperature
---------- Original Message ----------
>Hi i' am looking for the recipe for Burgundy Matte Raku glaze . Can anyone help?
Thanks
>Betsy Cox
>______________________________________________________________________________
>Send postings to clayart@lsv.ceramics.org
>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/
>Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.
Karen Shapiro on sun 4 aug 02
Here's what I have in my files:
"Burgundy Matt Raku"
Gerstley Borate 50, Talc 30, Nepheline Syenite 20, Copper Carb 3
(matt dark turguoise in oxidation, burgundy to orange in reduction)
Karen in Gualala
---------------------------------
Do You Yahoo!?
Yahoo! Health - Feel better, live better
Lori Richter on sun 4 aug 02
>Sent: Sunday, August 04, 2002 11:28 AM
>Subject: burgundy matte raku glaze
>
>
>Hi i' am looking for the recipe for Burgundy Matte Raku glaze . Can anyone
help? Thanks
>
>Betsy Cox
>
>
Betsy,
I recall seeing a "Matt Burgundy Red" here when I was looking for recipes
for our summer program at school:
http://www.dinoclay.com/info/glazes/degraku.html#glz0061
Hope this helps,
Lori
"As you slide down the banister of life,
may all the slivers be pointing the right direction."
~Irish Blessing~
| |
|