FYI, here is the original text about the glazes in the photo.
Michele Williams
You will see there this glaze
SPECKLES3134GREEN
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
FRIT 3134 27.60
Cryolite 7.40
BALL CLAY AK 26.70
Magnesium Carb Light 1.00
SILICA 37.20
Rutile 5.00
Red Iron Oxide 1.50
Copper oxide black 4.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
Seger Weight%
KNO 0.442 6.29%
CaO 0.441 5.67%
MgO 0.117 1.08%
Al2O3 0.460 10.74%
B2O3 0.405 6.47%
SiO2 4.674 64.41%
TiO2 0.291 5.34%
Na2O 0.442 6.29%
Al:Si 10.17
Expan. 7.49
ST 334.02
As it is on several claybodies
And you will say: Shame on you Ababi
You will see it as a part of my "combination", above this revised glaze. I
improved the
glaze by decreasing the feldspar adding frit that gave me room for more
kaolin that
was very low in the first recipe I used. Both recipes are good, according to
your raw
materials:
FOLLOW KOREN 27 1# (layer one)
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
Cone 6
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
SILICA 29.00
Calcium Carbonate 12.00
EPK Kaolin 14.00
ZINC OXIDE 10.00
Custer feldspar 13.00
STRONTIUM CARBONATE 7.00
FRIT 3110 15.00
And
FOLLOWS KOREN 27 #2 (layer one)
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
Cone 6
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
SILICA 31.50
Calcium Carbonate 12.00
EPK Kaolin 13.50
ZINC OXIDE 10.00
Nepheline Syenite 10.00
STRONTIUM CARBONATE 7.00
FRIT 3110 16.00
The glaze is very similar to Xavier , glossier.
You may try to add copper oxide 5'6,7, until it start being gray green,
than I belive will
be in its best
Merry glazing and happy poting