search  current discussion  categories  books & magazines - magazines 

can someone look up an article for me in ceramics monthly

updated wed 21 aug 02

 

Donn Buchfinck on sun 18 aug 02


I don't have this issue
December 1994
pg 32
called memphis mashiko stone
I am looking for the recipies

thanks
Donn Buchfinck

Hank Murrow on mon 19 aug 02


>I don't have this issue
>December 1994
>pg 32
>called memphis mashiko stone
>I am looking for the recipies
>
>thanks
>Donn Buchfinck

Dear Donn;

Is this what you are looking for?

Hank in Eugene

Glaze name: Fake Mashiko Kaki
Cone: 10
Color: klassic kaki
Testing: Untested
Surface texture: demi - gloss
Firing: Reduction
Glaze type: Mid Road Kaki

Recipe: Percent
Kona F-4 Soda Feldspar 36.27
Bone Ash 0.35
Talc 4.10
Wollastonite 5.47
Calcined Red Art Clay 37.76
Red Art Clay 3.97
Silica 8.60
red iron oxide 3.48
Totals: 100.00 % 40.00 Lb

Also add:
Darvan 811

Comments:
Good with chun or celadon variants; wax resist, etc.

Possible Health Hazards:
Talc: wear a NIOSH approved dust mask when handling dry material

Silica: free silica-wear a NIOSH approved dust mask when handling dry material

Unity Formula for Fake Mashiko Kaki:
0.196 K2O 0.731 Al2O3 5.826 SiO2
0.213 Na2O 0.197 Fe2O3 0.030 TiO2
0.332 CaO 0.006 P2O5 8.0:1 Si:Al Ratio
0.259 MgO

Percentage Analysis for Fake Mashiko Kaki:
67.31 % SiO2
14.33 % Al2O3
3.55 % K2O
2.54 % Na2O
3.58 % CaO
2.01 % MgO
6.05 % Fe2O3
0.16 % P2O5
0.46 % TiO2

John Weber on tue 20 aug 02


Oh, the one with cover boy, Richard Aerni:)
CM 1994 at p.32 shows:
Sohngen Kaki Glaze
Synthetic Bone Ash .36%
Talc 4.25
Wollastonite 5.67
Kona F-4 Feldspar 37.58
Calcined Cedar Heights
Redart 39.12
Cedar Heights Redart 4.11
Flint 8.91
Total 100%
Add: Iron Oxide 3.61%