search  current discussion  categories  techniques - misc 

trunks and textures

updated wed 21 aug 02

 

Ababi on tue 20 aug 02


http://members4.clubphoto.com/ababi306910/185990/
Slide one: SiC Slip And Glaze
1-5% Sic 100# in slip from the same claybody of the test tile above it some glazes
and the way they reacted to the SiC ^6 ox.

Slide leven to slide twenty: Texturals crwalings soda water and trunks

SUPERCRAWL AVERAGE 4
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

^6 Ox
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cryolite 15.00
ULTROX 35.00
BALL CLAY AK 9.00
Magnesium Carb Light 11.00
Nepheline Syenite 30.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.551 12.59%
CaO 0.013 0.26%
MgO 0.436 6.21%
Al2O3 0.430 15.47%
SiO2 1.826 38.75%
ZrO2 0.612 26.62%
TiO2 0.004 0.10%
K2O 0.047 1.56%
Na2O 0.504 11.03%
Al:Si 4.25
Expan. 8.31
ST 367.33
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
SUPERCRAWL #6
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,


Cone 6
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Nepheline Syenite 10.00
Magnesium Carb Light 3.66
BALL CLAY AK 3.00
Cryolite 25.00
ULTROX 58.33
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.813 14.17%
CaO 0.005 0.08%
MgO 0.181 2.03%
Al2O3 0.373 10.57%
SiO2 1.776 29.63%
ZrO2 1.271 43.49%
TiO2 0.001 0.03%
K2O 0.020 0.51%
Na2O 0.794 13.66%
Al:Si 4.75
Expan. 8.67
ST 345.52
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Please note: Go somewhere else when there is cryolite in the firing!
Ababi Sharon
Glaze addict
Kibbutz Shoval Israel
ababisha@shoval.org.il
http://members4.clubphoto.com/ababi306910/
http://www.milkywayceramics.com/cgallery/asharon.htm