here are the recipes to my new raku .

updated fri 23 aug 02

 

Ababi on thu 22 aug 02


Hello potters

Here are the recipes to my new raku .
All the recipes based on former 04 ox recipes I used or made myself all the way ( the
ash glaze) or most of the way or some way.
They are made out of various frits. You can buy all the frits in Israel. but you cannot
buy Cadycal here.
I made them with 3 copper ox or carb
You can try them with any colorants just add a bit of copper for flash can be 1%
The ash glaze does not have crackles.




CRACKLE ANAT 04 OX R
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 04 1060 deg.C. - Oxidation
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

FRIT A 2120 p 49.00
ENGLISH KAOLIN CC31 15.00
NORFLOAT POTASH FELDSPAR 10.00
SILICA 2.00
FRIT F-5 24.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.742 21.05%
CaO 0.258 6.18%
Al2O3 0.213 9.28%
B2O3 0.312 9.27%
SiO2 2.112 54.22%
K2O 0.102 4.09%
Na2O 0.640 16.97%
Al:Si 9.91
Expan. 12.12
ST 272.82
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

This is the crackled plate in my site
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
In the next test I will add 3% tin to emphasize the copper in the ware or the copper
spots



DELICATE OX AND RAKU
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 04 1060 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

FRIT VO 6004p 230.0
FRIT 3110 220.0
ENGLISH KAOLIN CC31 180.0
STRONTIUM CARBONATE 220.0
SILICA 150.0
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
plus colorants I used copper oxide 3 this is the mushroom ware in my site

Seger Weight%
KNO 0.456 11.65%
CaO 0.078 1.53%
SrO 0.466 16.94%
Al2O3 0.250 8.93%
B2O3 0.289 7.07%
SiO2 2.554 53.88%
K2O 0.152 5.03%
Na2O 0.304 6.62%
Al:Si 10.23
Expan. 9.51
ST 332.32
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

LOW MOTTLED ASH OX RAKU
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 04 1060 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

FRIT 3701 300.0
PINE ASH 200.0
BALL CLAY AK 200.0
Wollastonite 50.00
ULTROX 150.0
FRIT A 2120 p 100.0
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
I used as white and as with copper

Seger Weight%
KNO 0.481 14.65%
CaO 0.354 8.23%
MgO 0.113 1.88%
Li2O 0.053 0.66%
Al2O3 0.176 7.43%
P2O5 0.032 1.89%
B2O3 0.417 12.03%
SiO2 1.698 42.34%
ZrO2 0.209 10.69%
TiO2 0.006 0.21%
K2O 0.171 6.68%
Na2O 0.310 7.97%
Al:Si 9.66
Expan. 9.38
ST 294.44
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
this is the small jar in my site

SOFT RAKU
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 04 1060 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

FRIT 3110 180.0
FRIT 3134 300.0
ENGLISH KAOLIN CC31 200.0
SILICA 120.0
Cryolite 140.0
Cadycal (California) 60.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.572 14.38%
CaO 0.427 9.47%
MgO 0.001 0.02%
Al2O3 0.308 12.41%
B2O3 0.409 11.26%
SiO2 2.208 52.47%
K2O 0.029 1.07%
Na2O 0.543 13.31%
Al:Si 7.17
Expan. 10.37
ST 305.64
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Comment: This is the Lana Wilson's stile vase in my site