search  current discussion  categories  glazes - cone 8-10 

ame glaze recipe cone 9-10

updated fri 30 aug 02

 

June Perry on thu 29 aug 02


Here's a recipe from my glaze database. You will probably want to eliminate
the lead! I don't know if this was an oxidation or reduction glaze. I may be
intended for oxidation???

#1274 AME GLAZE C 9 - 10

OXFORD SPAR 34.57
WHITING 10.27
KAOLIN 8.46
FLINT 16.52
MAGNESITE .18
COMMON ASH 25.00
RED LEAD 5.00

ADD: RED IRON OXIDE 8%

Regards,
June Perry