glaze test for malcolm david shino, cone 10 redux, fired to cone 6 ox.

updated mon 9 sep 02

 

Alisa Liskin Clausen on sun 8 sep 02


Glaze test for Malcolm Davis Shino, cone 10 redux., fired to cone 6, ox.
Glaze tested on white midrange stoneware fired in electric oxidation to =
1220c.

Source: Clayart
Credited to: Malcolm Davis

Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1100c (330f - 2012f)=20
100c p/h to 1220c (212f - 2228f)
cool down max. per hour to 1100c=20
cool 80c per hour to 800c
shut off kiln

Recipe:

40.91 Neph. Syenite
17.27 Soda Ash
9.82 Kona F4 Soda spar
18.18 EPK
13.82 OM4

Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in percent =
to the 100 gram test batch.

Substitutions:
Added 10% Borax Frit to above recipe.

Results:
All white, thick, covering shino glaze. Crazed.

Regards from Alisa in Denmark