Alisa Liskin Clausen on sun 8 sep 02
Glaze test for Satin Spodumene cone 6 redux, fired to cone 6 ox.
Glaze tested on white midrange stoneware fired in electric oxidation to =
1220c.
Source: Clayart
Credited to:
Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1100c (330f - 2012f)=20
100c p/h to 1220c (212f - 2228f)
cool down max. per hour to 1100c=20
cool 80c per hour to 800c
shut off kiln
Recipe:
28.57 Spodumene
22.86 Dolomite
20.0 Custer
11.43 Silica
8.57 Kaolin
4.76 Zircopax
3.81 Gerstely Borate
Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in percent =
to the 100 gram test batch.
Substitutions:
Local feldspar for Custer
Borax frit for Gerstley Borate
Results:
White semi matte glaze with some glossier streaking. Covering.
Regards from Alisa in Denmark
Ron Roy on thu 12 sep 02
This glaze may be stable - expansion is such that it will not craze on many
clay bodies.
RR
>Glaze test for Satin Spodumene cone 6 redux, fired to cone 6 ox.
>Glaze tested on white midrange stoneware fired in electric oxidation to 1220c.
>
>Source: Clayart
>Credited to:
>
>Firing ramp:
>100c p/h to 600c (212f - 1112f)
>150c p/h to 1100c (330f - 2012f)
>100c p/h to 1220c (212f - 2228f)
>cool down max. per hour to 1100c
>cool 80c per hour to 800c
>shut off kiln
>
>Recipe:
>28.57 Spodumene
>22.86 Dolomite
>20.0 Custer
>11.43 Silica
>8.57 Kaolin
>4.76 Zircopax
>3.81 Gerstely Borate
>
>
>Note: All raw materials are measured up or down to the nearest whole
>decimal.
>Colorants or additives to a 100 gram test batch are measured in percent to
>the 100 gram test batch.
>
>Substitutions:
>Local feldspar for Custer
>Borax frit for Gerstley Borate
>
>Results:
>White semi matte glaze with some glossier streaking. Covering.
>
>Regards from Alisa in Denmark
>
>______________________________________________________________________________
>Send postings to clayart@lsv.ceramics.org
>
>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/
>
>Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.
Ron Roy
RR#4
15084 Little Lake Road
Brighton, Ontario
Canada
K0K 1H0
Phone: 613-475-9544
Fax: 613-475-3513
| |
|