search  current discussion  categories  glazes - cone 4-7 

glaze test for shino cone 6 redux. fired to cone 6 ox.

updated mon 9 sep 02

 

Alisa Liskin Clausen on sun 8 sep 02


Glaze test for Shino cone 6 redux, fired to cone 6 ox.

Glaze tested on white midrange stoneware fired in electric oxidation to =
1220c.

Source: Clayart
Credited to:

Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1100c (330f - 2012f)=20
100c p/h to 1220c (212f - 2228f)
cool down max. per hour to 1100c=20
cool 80c per hour to 800c
shut off kiln

Recipe:
54.5 Neph. Syenite
22.8 Spodumene
14.9 Ball Clay
4.9 Gerstely Borate
2.9 Soda Ash

Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in percent =
to the 100 gram test batch.

Substitutions:
Borax frit for Gerstely Borate

Results:
White, covering Shino glaze, crazed.

Regards from Alisa in Denmark