This is the one glaze I did not investigate all the way, but I think it can be a very good
raku glaze. Not a crackle glaze.


LOW ALUMINA JADE A Raku ash glaze
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 08 945 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

PINE ASH 10.00 .....barbecue ash
FRIT A 2120 p 35.00
FRIT VO 6004p 35.00
ULTROX 10.00
SILICA 10.00
Copper Carbonate 3.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.764 22.95%
CaO 0.199 4.74%
MgO 0.037 0.64%
Al2O3 0.053 2.28%
P2O5 0.015 0.90%
B2O3 0.306 9.05%
SiO2 2.059 52.62%
ZrO2 0.130 6.82%
K2O 0.204 8.19%
Na2O 0.560 14.75%
Al:Si 39.18
Expan. 11.94
ST 253.61

The name means only the source of this recipe, ^04 oxidation ash - lithium glaze of
Eduard B.. It gives rich red brown on my porcelain claybodies.
You may get it on any raku claybody if you use a slip rich with of English Kaolin CC31
locally used which is very white,on the greenware,

I tried hardly to convert it to the "west side" materials and failed. The only way was to
use soluble materials.
Frit 2120 can be replaced ( through a software) to 3110
6004 is quite similar to frit F 74
I know from Tom Buck that to order it you must order a sack.
I, me, Ababi the glaze addict would not order a sack to test a new glaze.
Ababi Sharon
Glaze addict
Kibbutz Shoval Israel
ababisha@shoval.org.il
http://members4.clubphoto.com/ababi306910/
http://www.milkywayceramics.com/cgallery/asharon.htm