c10 black matt recipe enclosed

updated tue 17 sep 02

 

June Perry on sat 14 sep 02


A while back someone askef for a cone 10 black matt. While going through my
database this one came up. My test was a lovely satin matt.

#215 J.BOBBS MATT BLACK C10 REDUCTION/ OXIDATION

POTASH FELDSPAR 5584.8
WHITING 568.9
CHINA CLAY 1526.4

ADD: COBALT OXIDE 221.76, IRON OX IDE 253.5

Regards,
June

Ron Roy on mon 16 sep 02


The alumina content is very high so I assume this glaze is not completely
melted - if not it will release colour very easily.

I went to art school with J Bobbs - she must be getting on too.

RR


>A while back someone askef for a cone 10 black matt. While going through my
>database this one came up. My test was a lovely satin matt.
>
>#215 J.BOBBS MATT BLACK C10 REDUCTION/ OXIDATION
>
>POTASH FELDSPAR 5584.8
>WHITING 568.9
>CHINA CLAY 1526.4
>
>ADD: COBALT OXIDE 221.76, IRON OX IDE 253.5
>
>Regards,
>June

Ron Roy
RR#4
15084 Little Lake Road
Brighton, Ontario
Canada
K0K 1H0
Phone: 613-475-9544
Fax: 613-475-3513