Base Glaze #2
Ferro Frit #3195 88.24%
China Clay (EPK) 11.76%
Total 100%

Turquoise
Base Glaze #2 100%
add copper oxide 1.47%
Superpax 4.90%


Ann -in the south west regions of Vancouver Island off the coast of British
Columbia, Canada, surrounded by evergreens, clean air, and two muddy messy
dogs and two demented cats.
annsemple@shaw.ca

iandol on wed 9 oct 02


Dear Ann Semple,

You say < This is the recipe from Trevor Youngberg's article on =
Programmable low fire glazes in the May/June Clay times.>

Not all of us are fortunate to have access to this magazine. So please =
enlighten us. What are "Programmable low fire glazes" ?

Is this a new breed or recipes or is it to do with using a kiln =
controller? If it is the latter, then it would seem that instructions =
are required to obtain the designed effects.

Best regards,
Ivor Lewis. Redhill, South Australia.