search  current discussion  categories  materials - clay 

rudolf staffel clay body tips

updated sat 9 nov 02

 

David Beumee on thu 7 nov 02


I'd be happy to give you some recipes, but have you tried Southern Ice, sold by Laguna?
My testing shows excellent whiteness, fired to cone 11, and a beautiful throwing porcelain body
as well, meaning that it's rather easy to throw it thin enough to get translucency.

David Beumee
Earth Alchemy Pottery
Lafayette, Colorado





11/7/02 10:04:54 AM, Adams Robertson Puryear wrote:

>Hi, I am trying to make a translucent porcelaneous
>clay body much like Rudy Staffel's Light Gatherer
>series. Any help would be appreciated, thankyou.
>
>
>
>
>__________________________________________________
>Do you Yahoo!?
>U2 on LAUNCH - Exclusive greatest hits videos
>http://launch.yahoo.com/u2
>
>______________________________________________________________________________
>Send postings to clayart@lsv.ceramics.org
>
>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/
>
>Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.
>

Adams Robertson Puryear on thu 7 nov 02


Hi, I am trying to make a translucent porcelaneous
clay body much like Rudy Staffel's Light Gatherer
series. Any help would be appreciated, thankyou.




__________________________________________________
Do you Yahoo!?
U2 on LAUNCH - Exclusive greatest hits videos
http://launch.yahoo.com/u2

karen gringhuis on fri 8 nov 02


Adams -
My understanding is that Staffel's recipe(s) are "out
there" - perhaps published in CM or from a former
student at Tyler?

Meanwhile, here's a recipe which might meet your needs
or provide info.

Grolleg 20%
EPK 8
Tile #6 8
Kona F-4 38
Whiting 4
Flint 22
total 100%
Macaloid 3%

He may have added a little molochite or alumina.
Your challenge is to acheive translucency without
slumping. I have no idea if RS ever fired his pieces
in a mold for support.

Good luck and please post any test results.







=====
Karen Gringhuis
KG Pottery
Box 607 Alfred NY 14802

__________________________________________________
Do you Yahoo!?
U2 on LAUNCH - Exclusive greatest hits videos
http://launch.yahoo.com/u2