search  current discussion  categories  kilns & firing - construction 

kiln repair/itc/fiber

updated thu 14 nov 02

 

mel jacobson on wed 13 nov 02


one of the neatest ways to get your cover to fit, repair small
holes in your kiln...or just plain stuff a crack.

take kaowool and mash it up....then add
itc 100 to make a paste.
push the paste/kaowool into the crack or hole.
fire kiln...repaired.

you could even out the top of an electric with this mix.
it will not shed fiber.
after the kiln is fired, it will be hard as rock.

itc stabilizes fiber. i often think it is it's best feature.
mel
From:
Minnetonka, Minnesota, U.S.A.
web site: my.pclink.com/~melpots
or try: http://www.pclink.com/melpots