Alisa Liskin Clausen on sat 16 nov 02
ox.
Glaze test for oxides under zinc Semimatte/Glossy Base Glaze, cone 6, =
ox.
Glaze tested on white midrange stoneware fired in electric oxidation to =
1220c.
Source: Mastering Cone 6 Glazes
Credited to: John Hesselberth and Ron Roy
Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1100c (330f - 2012f)=20
100c p/h to 1220c (212f - 2228f)
cool down max. per hour to 1100c=20
cool 80c per hour to 800c
shut off kiln
Recipe:
Please refer to the above book page 98.
Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in percent =
to the 100 gram test batch.
Substitutions:
Results:
Smooth semi gloss white glaze.=20
Oxides Cobalt, RIO, black stain, Chrome and Ocher showed well under =
glaze. The Cobalt is variegated with very slightly diffused edges. The =
Other oxides stayed where painted. The Chrome turned pinkish beige.