search  current discussion  categories  techniques - majolica 

majolica recipes

updated tue 24 dec 02

 

wynne wilbur on mon 23 dec 02


Linda Arbuckle majolica - Cone 03

Frit 3124 65.75
F-4 Feldspar 17.24
EPK 10.82
Neph Sy 6.24
Tin Oxide 5.0
Zircopax 10.0
Bentonite 2.0
Epsom salt to flocculate 1-3 tsp/5 gal

Smooth white surface. Colorants usually applied in a thin wash to raw glaze
surface. Does not move in firing. May crawl if thick or pinhole over rough
surfaces.

Anderson Majolica - cone 04-03

Frit 3124 55
OM4 Ball clay 10
Flint 10
Zircopax 8




Hope these help. I have many others if you are interested.