^6 soda

updated sat 25 jan 03

 

lyla kaplan on fri 24 jan 03



mark,


julia galloway does ^6 soda and she gets great results. i have done a little bit of experimenting at home, but have a long way to go.


below are glazes and slips she gave us at a workshop.  please email me offline if you want to talk more...


good luck


lyla


Glazes from Julia Galloway – Arrowmont, 2000


 


^6 soda, light redux


 


Alec Karros for Color Base


 


Kona F-4         11


Neph sye         21


Gerst Borate   10


Whiting            4


Wollastonite    8


Barium Carb   12


EPK                 10


Flint                 35


 


To 100g of base:


Red: 10% Degussa red


            5% red iron ox


 


Orange:  10% degussa orange


            1% rutile


 


Yellow: 10% bright yellow stain (goes pale in reduction)


 


Black: 8% black stain


            2% barnard (rim may go blue)


 


Stoive Halo Matt Poison Beauty


 


Neph Sye        60


Barium carb    22


Lithium carb    5


Ball clay           7


Flint                 6


Vanadium pentoxide


                        5


 


halo created on clay body


 


Mang Luster


 


Redart             60


Mang Diox       45


Ball clay           5


Flint                 5


Cobalt              10


Copper            10


 


Very smokey black with coppery luster.


 


Rutile Ash


 


Custer             14


Barium                        9


Dolomite          9


Whiting            26


Ball clay           20


Flint                 18


Rutile               6


Gerst Borate   12


 


Very runny, range tan/yellow/peach.


 


Don’t put on top of any other glaze.


 


Silverman Blue (Persian blue)


 


g-200 feldspar 45


whiting             7


Grolleg             6


Flint                 7


Barium                        35


Copper            8


 


When in doubt, use this. Satin matt wax doesn’t resist. Goes on top of ash


 


Hamada base revised (runs)


 


Custer             53


Whiting            9


Zinc                 9


Barium                        21


Ball clay           1


Gerst borate    10


 


Light blue: 2% copper


 


Bright green (grass): 6% copper


 


Emerald green (dark):


            Rutile    2


            RIO       2


            Copper 3


 


  



Slips ^5-7


 


Black slip


 


Tenn ball clay  40


Neph sye         10


Wollostonite    10


Black 6600      25


 


 


Green slip


 


Tenn ball         40


Neph sye         30


Wollostonite    5


Silica               10


Fr green 6219 15


 


Blue slip


 


Tenn ball         40


Neph sye         30


Wollastonite    10


Silica               10


Cobalt carb     10


 


 


Yellow slip


 


Tenn ball         40


Neph sye         12.5


Wollastonite    5


Praes Yel 6450  25


 


****BARIUM IS POISONOUS


NOT FOR FOOD SURFACES






          


      imagine


          




>From: Automatic digest processor
>Reply-To: Clayart
>To: Recipients of CLAYART digests
>Subject: CLAYART Digest - 22 Jan 2003 to 23 Jan 2003 (#2003-24)
>Date: Fri, 24 Jan 2003 00:00:00 -0500
>
><< multipart1 >>


STOP MORE SPAM with the new MSN 8 and get 2 months FREE*