search  current discussion  categories  materials - frits 

frit substitue for xavier's warm jade green i was sleepy >3195

updated wed 29 jan 03

 

Ababi on tue 28 jan 03


Sorry I was sleepy

XAVIER 3195
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Custer feldspar 30.00
frit 3195 16.90
Calcium Carbonate 15.60
talc Nital 8.80
EPK Kaolin 17.60
silica 11.20
Rutile 5.00
Copper carbonate 4.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.194 5.33%
CaO 0.606 11.92%
MgO 0.200 2.82%
Al2O3 0.408 14.56%
P2O5 0.001 0.04%
B2O3 0.167 4.08%
SiO2 2.654 55.91%
TiO2 0.191 5.34%
K2O 0.099 3.25%
Na2O 0.096 2.08%
Al:Si 6.51
Expan. 7.52
ST 372.24
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Clay Body
Colour
Glaze Type
Opacity
Texture
Stability
Fit
Last changed:
Status
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
Comment: No comment!

Ababi Sharon
Glaze addict
Kibbutz Shoval Israel
ababisha@shoval.org.il
http://members4.clubphoto.com/ababi306910/
http://www.milkywayceramics.com/cgallery/asharon.htm
and also
http://www.israel-ceramics.org/membersGallery/personalpage.asp?MID=507