Coleman's recipe for P.D. Shino Crack:

8 Custer
11 Spodumene
3 Soda Ash
26 EPK
37 Neph Sy
11 OM-4
4 Magnesium carb

" Stiff surface if applied thickly; will crack apart and expose the
surface beneath. Great over dark stoneware or over dark slips on
porcelain. Will not shift or run at cone 10. Cone 9-10 reduction."


David Beumee







2/6/03 8:55:06 AM, Chris Rupp wrote:

>Hello,
>
>A while back I remember seeing a recipe named "PD CRACK - SHINO," in Tom
>Coleman's, "The Glazes I Use." I don't have the book and was hoping someone
>might have it and be willing to share the recipe with me. If so you can
>email it to me at: cmrdesigns@hotmail.com
>
>THANK YOU FOR YOUR TIME!
>
>Chris Rupp
>Sunny Santa Barbara
>
>_________________________________________________________________
>MSN 8 with e-mail virus protection service: 2 months FREE*
>http://join.msn.com/?page=features/virus
>
>______________________________________________________________________________
>Send postings to clayart@lsv.ceramics.org
>
>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/
>
>Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.
>

Chris Rupp on thu 6 feb 03


Hello,

A while back I remember seeing a recipe named "PD CRACK - SHINO," in Tom
Coleman's, "The Glazes I Use." I don't have the book and was hoping someone
might have it and be willing to share the recipe with me. If so you can
email it to me at: cmrdesigns@hotmail.com

THANK YOU FOR YOUR TIME!

Chris Rupp
Sunny Santa Barbara

_________________________________________________________________
MSN 8 with e-mail virus protection service: 2 months FREE*
http://join.msn.com/?page=features/virus