chrome tin reds 0.35% chrom of course!

updated mon 10 mar 03

 

Ababi on sun 9 mar 03


0.35% chrom of course!
---------- Original Message ----------

>Yes I think I had tried it was fine, not a celebration.
>I tested some of mine too some "grids" and some line blends.
>I think the one here was the best ( To my test)
>ABABI WOLLASTONITE BASE MAUVE
>,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

>Cone 6 1222 deg.C. -
>,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

>kaolin CC31 20.00
>Wollastonite 34.00
>Feldspar Soda F7 32.00
>frit A 2120 7.00
>kaolin CC31 calcined 7.00
>Tin Oxide 7.00
>Chrome Oxide 3.50
>,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,


>,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
>The nearest to your materials will be
>ABABI WOLLASTONITE BASE MAUVE W
>,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

>Cone 6 1222 deg.C. -
>,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

>Custer feldspar 53.80
>OM-4 Ball Clay 20.20
>Dolomite 0.70
>Calcium Carbonate 17.60
>Wollastonite 7.60
>Tin Oxide 7.00
>Chrome Oxide 3.50
>,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,