search  current discussion  categories  glazes - specific colors 

glaze tests results: ababi's glossy almost turquoise

updated mon 24 mar 03

 

Ababi on mon 24 mar 03


Hi!
I tried to sub some materials in my S4b.
I failed but got nice results:
I got in both tests very similar results. Glossy shiny pale turquoise or green. In one of
the tests, where was thick was mottled ( in the imprints)
Here are both recipes for your use. I will rename the glaze according to the results:
They asked the bowman: "How do all your arrows are always in the
middle of the circle?" I shoot first and than paint the circle around"! Said the bowman!
GLOSSY Almost TURQUOISE 2
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Quartz 13.70
EPK Kaolin 22.90
strontium carbonate 15.50
Wollastonite 13.60
frit 3110 29.50
Alumina Hydrate 4.80
Tin Oxide 5.00
copper oxide 3.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.247 5.27%
CaO 0.415 7.65%
MgO 0.015 0.20%
SrO 0.322 10.95%
Al2O3 0.408 13.64%
B2O3 0.034 0.77%
SiO2 3.112 61.42%
TiO2 0.003 0.09%
K2O 0.022 0.69%
Na2O 0.225 4.58%
Al:Si 7.63
Expan. 7.80
ST 372.46

,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
Comment: White stoneware or porcelain


ABABI'S GLOSSY Almost TURQUOISE CUSTER&EPK
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Custer feldspar 48.70
EPK Kaolin 10.20
Wollastonite 15.80
strontium carbonate 14.10
silica 11.20
Tin Oxide 5.00
copper oxide 3.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.255 6.82%
CaO 0.406 7.25%
MgO 0.020 0.25%
SrO 0.320 10.56%
Al2O3 0.411 13.33%
SiO2 3.227 61.75%
TiO2 0.002 0.04%
K2O 0.175 5.25%
Na2O 0.080 1.57%
Al:Si 7.85
Expan. 7.77
ST 373.35
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
I prefer the second one because of the lower cost

I will go on trying because I have only 5 K'g left of cryolite
I think a Currie grid out of Behrens's stony white/ green might help.
I am waiting to the pictures. When I will get them I will show them.