search  current discussion  categories  glazes - cone 4-7 

glaze test for edwards chrome tin, november version, cone 6, oxidation.

updated wed 30 apr 03

 

Alisa Clausen on tue 29 apr 03


Glaze test for Edwards Chrome Tin, November Version, cone 6, oxidation.

Glaze tested on white midrange stoneware fired in electric oxidation to =
1220c.

Source:
Credited to:

Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1100c (330f - 2012f)=20
100c p/h to 1220c (212f - 2228f)
5 min. soak
cool down 80c per hour to 800c
shut off kiln

Recipe:

25 Neph. Syenite (Blue Mountain)
20 Wollastonite
15 Frit 3134
15 Silica
5 Talc

ADD
0,30 Chromium Oxide Green
6.0 Tin Oxide

Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in percent =
to the 100 gram test batch.

Substitutions:
Local Neph. Syenite for Blue Mountain.

Results:

Regards from Alisa in Denmark