ox.
Glaze test for Raspberry (Mastering Cone 6 Glazes) as Purple, cone 6, =
ox.
Glaze tested on white midrange stoneware fired in electric oxidation to =
1220c.
Source: MC6G and Clayart revision.
Credited to:
Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1100c (330f - 2012f)=20
100c p/h to 1220c (212f - 2228f)
5 min. soak
cool down 80c per hour to 800c
shut off kiln
Recipe:
See Mastering Cone 6 Glazes
Hesselberth/Roy
Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in percent =
to the 100 gram test batch.
Substitutions:
Frit 623 for 3134
Added
1.0 Cobalt Carb.
0.25 RIO
(instead of Chrome/Tin ox.)
Results:
Gloss blue glaze that has many variations on a smooth. Lush covering =
with streaking and movement. =20
Glaze at bottom edge thickened but did not run. =20
Regards from Alisa in Denmark
| |
|