search  current discussion  categories  glazes - cone 8-10 

cone 10 crater- lava glaze formulation?

updated wed 14 may 03

 

Adam Rubinstein on mon 12 may 03


Hello,


I am looking for a good cone 10 glaze recipie that produces craters, soft
rounded ones preferably.

Any hints?

Ababi on tue 13 may 03


Try to add to a matte glaze 1-2% silicon carbide 100#
or apply a slip out of the claybody you use with1- 2% SiC and after bisque add a
matte glaze.
Test first because each base acts differently.
See in my glaze tests page (^6 ox.)
By it from an abrasive store
Ababi Sharon
Glaze addict
Kibbutz Shoval Israel
ababisha@shoval.org.il
http://members4.clubphoto.com/ababi306910/
http://www.milkywayceramics.com/cgallery/asharon.htm
---------- Original Message ----------

>Hello,


>I am looking for a good cone 10 glaze recipie that produces craters, soft
>rounded ones preferably.

>Any hints?

>______________________________________________________________________________
>Send postings to clayart@lsv.ceramics.org

>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/

>Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.