Glaze test for Berry Rust, cone 6, ox. Revsion.
Glaze tested on white midrange stoneware fired in electric oxidation to =
1220c.

Source:
Credited to:

Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1100c (330f - 2012f)=20
100c p/h to 1220c (212f - 2228f)
5 min. soak
cool down max. to 800c
Hold 1 hour
Shut off kiln

Recipe:
26 Silica
27 EPK
7 Nepheline Syenite
9 Bone Ash
13 Talc
18 Frit 3134

ADD
12 RIO

Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in precent =
to the 100 gram test batch.

Substitutions: None

Results:
Gloss iron red glaze. Well covering and smooth. Darker where thinner =
or breaking, lusher red iron red color where thickest. =20

Regards from Alisa in Denmark