Dannon Rhudy on tue 1 jul 03


Connie said:

> I'm having a real problem reglazing part of a pot
........repels reglazing, .> Any suggestions will be greatly
appreciated....>>>

You don't say if the piece has already been fired, or if
there is simply a small chip in the un-fired glaze. If it's
been fired, you can mix a small amount of wallpaper paste
into your glaze. It must be a very small amount, and only
mix it into the glaze you intend to use. Throw out leftovers.

If the piece is not yet fired, mix any sticky substance into
your glaze (white glue, syrup, etc) and brush the glaze onto
the chipped place. If there is WAX on the unglazed part,
then you need to wash the piece, sand off the wax, and
start over.

regards

Dannon Rhudy
>
> Thanks.
> Connie, in Atlanta where the rain just keeps coming down.
>
> _________________________________________________________________
> MSN 8 helps eliminate e-mail viruses. Get 2 months FREE*.
> http://join.msn.com/?page=features/virus
>
>
____________________________________________________________________________
__
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.
>

Connie Stockdale on tue 1 jul 03


I'm having a real problem reglazing part of a pot where the glaze has been
chipped off. Since it was a complicated hot wax pattern resist kind of
thing, I really would like to salvage the pot. The problem is that the
glaze is shino, the recipe containing about 65% nepheline syenite. The soda
ash seems to leave a residue that repels reglazing, even with the original
shino. Would a little Vee-Gum in a small amount of glaze help it to adhere?
Any suggestions will be greatly appreciated.

Thanks.
Connie, in Atlanta where the rain just keeps coming down.

_________________________________________________________________
MSN 8 helps eliminate e-mail viruses. Get 2 months FREE*.
http://join.msn.com/?page=features/virus

Carol Tripp on wed 2 jul 03


Try some wallpaper paste mixed into the glaze. It drys on like a rock.
Good luck,
Carol
Dubai, UAE

Connie wrote:
>I'm having a real problem reglazing part of a pot where the glaze has been
>chipped off. Since it was a complicated hot wax pattern resist kind of
>thing, I really would like to salvage the pot. The problem is that the
>glaze is shino, the recipe containing about 65% nepheline syenite. The
>soda
>ash seems to leave a residue that repels reglazing, even with the original
>shino. Would a little Vee-Gum in a small amount of glaze help it to
>adhere?
> Any suggestions will be greatly appreciated.
>
>Thanks.
>Connie, in Atlanta where the rain just keeps coming down.
>

_________________________________________________________________
MSN 8 with e-mail virus protection service: 2 months FREE*
http://join.msn.com/?page=features/virus

Lee Love on wed 2 jul 03


Connie,

I'm guessng that you are trying to reglaze an unfired pot where you
scraped wax off of the bisque to reglaze? If so, and the residual wax is a
problem, use a torch or paint stripper to burn the wax off (you can also hold
the area in front of the peep of a firing kiln.)

If the pot has been fired alread and you want to fill in a chipped area,
scrape some glaze off of the wall of the glaze bucket above the glaze level, and
take this paste and "inlay" it in the hole. This can also be done when
refiring pinholing: fill in the holes with glaze paste and then dip the whole
pot in glaze. It is best if you warm the pot up a bit first.

--
Lee Love in Mashiko, Japan