search  current discussion  categories  materials - frits 

sub. for fritt p311

updated fri 4 jul 03

 

Susan Fortuna on thu 3 jul 03


I work with majolica glazes and need a subsitute for P311 glaze. I was told
that frit 3124 would be good. Before I mix it I would like someone to confirm
that since I will be mixing a large bach.

Ababi on thu 3 jul 03


Hello Susan
For 100% of P311
Use:
P311 SUB
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Ferro 3134 59.30
Custer feldspar 5.20
EPK 22.90
Calcium Carbonate 2.70
Flint 10.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.308 7.13%
CaO 0.692 14.09%
Al2O3 0.271 10.02%
B2O3 0.570 14.41%
SiO2 2.491 54.36%
K2O 0.016 0.55%
Na2O 0.292 6.58%
Al:Si 9.20
Expan. 8.07
ST 314.06
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
Ababi Sharon

Glaze addict

Kibbutz Shoval Israel

ababisha@shoval.org.il

http://members4.clubphoto.com/ababi306910

http://www.matrix2000.co.nz/Matrix%20Demo/Ababi.htm


-----Original Message-----
From: Clayart [mailto:CLAYART@LSV.CERAMICS.ORG] On Behalf Of Susan
Fortuna
Sent: Thursday, July 03, 2003 6:03 PM
To: CLAYART@LSV.CERAMICS.ORG
Subject: Re: Sub. for Fritt P311

I work with majolica glazes and need a subsitute for P311 glaze. I was
told
that frit 3124 would be good. Before I mix it I would like someone to
confirm
that since I will be mixing a large bach.

________________________________________________________________________
______
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.