search  current discussion  categories  glazes - misc 

nutmeg glaze (opps)

updated thu 21 aug 03

 

Rick on wed 20 aug 03


Sorry, I forgot to include the Satin Matte glaze I use. It comes from
CM June/July/August 1989 p. 97

Reduction
Cone 8 - 10

Dolomite------------- 20
Feldspar------------- 40
Kaolin --------------- 20
Flint ------------------ 20

Add:
Manganese ----- 1.0