search  current discussion  categories  techniques - cracking 

mending cracks with papooze

updated tue 21 oct 03

 

Alisa Clausen on sun 19 oct 03


You can use some of Peggy's Spooze and it with paper slip.
Here is the recipe for Paper Spooze, or now fondly called Papooze:

1 part Vinegar
2 parts Sugar or honey
3 parts Clay (Ball or your mix)
1 part Paper fibers, saturated and strained for water
mix to a thick consistency.

Mix up and use like repair slip.

regards from Alisa in Denmark
remembering Peggy.