search  current discussion  categories  glazes - misc 

glaze of week for oct 18.

updated sun 26 oct 03

 

Hal Mc Whinnie on thu 23 oct 03


f-4 spar 46.7
silica 15.2
talc 13.7
colemanite 11.65
dolomite 8.09
epk 4.5

alfred off white
cone 6
semi gloss
not fluid
statins show
white where thick

Jon Brinley on thu 23 oct 03


Sounds familiar

----- Original Message -----=20
From: Hal Mc Whinnie=20
To: CLAYART@LSV.CERAMICS.ORG=20
Sent: Thursday, October 23, 2003 2:31 PM
Subject: glaze of week for oct 18.


f-4 spar 46.7
silica 15.2
talc 13.7
colemanite 11.65
dolomite 8.09
epk 4.5

alfred off white
cone 6
semi gloss
not fluid
statins show
white where thick

=
_________________________________________________________________________=
_____
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at =
melpots@pclink.com.

Ron Roy on sat 25 oct 03


This glaze - on the other hand looks like a winner - I calculated it using
Gerstley borate rather than colmanite - it would not be hard to convert it
over to a borax frit - like 3134 for instance.

It's a high magnesia glaze by the way so look for that "buttery feel" and
maybe even cobalt giving purple blue.

Expansion is low enough that it will not craze on many cone 6 bodies -
silica and alumina are high enough that it will probably test out to be a
stable glaze.

If anyone wants to try converting it to 3134 I'll be glad to hold your hand.

RR


>f-4 spar 46.7
>silica 15.2
>talc 13.7
>colemanite 11.65
>dolomite 8.09
>epk 4.5
>
>alfred off white
>cone 6
>semi gloss
> not fluid
>statins show
>white where thick

Ron Roy
RR#4
15084 Little Lake Road
Brighton, Ontario
Canada
K0K 1H0
Phone: 613-475-9544
Fax: 613-475-3513

Edouard Bastarache Inc. on sat 25 oct 03


Ron,

using Colemanite in the original recipe :

Kona A3 12.58
Quartz 15.25
Talc 16.74
Whiting 0.08
Dolomite 4.66
EPK 18.66
Frit 3134 23.24
Frit 3110 8.78

assuming I have a little Gerstley left:

Kona A3 14.42
Quartz 16.05
Talc 16.44
Gerstley 10.39
Dolomite 2.25
EPK 16.88
Frit 3134 12.78
Frit 3110 10.79

using Gerstley in the original recipe :

Kona A3 20.42
Quartz 14.79
Talc 17.16
Whiting 1.48
Dolomite 6.12
EPK 15.36
Frit 3134 9.55
Frit 3110 15.11


Later,




"Ils sont fous ces quebecois"
Edouard Bastarache
Irreductible Quebecois
Indomitable Quebeker
Sorel-Tracy