Guy Watson on sat 29 nov 03
I live in Norway. We have a limited supply of frits. I am trying
substitutions but need more infor about the frit. Does anyone know who
produces the following frits?
Norwegian Frits (amounts first)
R76 Alkalifritte (1000-1200c) [Alkaline frit]
0.213 K2O
0.787 CaO
0.428 Al2O3
0.935 B2O3
3.275 SiO2
1048 Alkalifritte [Alkaline frit]
0.633 Na2O
0.293 K2O
0.006 MgO
0.067 CaO
0.783 Al2O3
0.876 B2O3
2.313 SiO2
2275 Alkalifritte (860-1060oc) [Alkaline Frit]
0.50 Na2O
0.33 K2O
0.17 CaO
0.10 Al2O3
0.10 B2O3
1.50 SiO2
H19 Bly monosilikat (880-1080) [Lead monosilicate frit]
1.00 PbO
0.047 Al2O3
0.603 SiO2
P29 Bly-bi-silikat (900-1100c) [Lead bisilicate frit]
1.00 PbO
0.086 Al2O3
1.86 SiO2
2262 Bly halvannensilicat (880.1080) [no translation] frit
1.00 PbO
0.125 TiO2
1.540 SiO2
MOK 3 Boraksfritte (780-1000c) [Borax frit]
0.417 Na2O
0.214 K2O
0.366 CaO ,
0.002 MgO
0.205 Al2O3
0.452 B2O3
1.884 SiO2
1047 Boraksfritte [ Borax frit]
0.369 Na2O
0.074 K2O
0.556 CaO
0.506 Al2O3
0.848 B2O3
1.955 SiO2
2263 Standard boraksfritte [ Standard borax frit]
0.330 Na2O
0.033 K2O
0.634 CaO
0.003 MgO
0.173 Al2O3
0.630 B2O3
1.880 SiO2
2270 Hvit zircon Boraks fritte [White zircon borax frit]
0.414 Na2O
0.061 ZnO
0.413 CaO
0.112 MgO
0.236 Al2O3
0.827 B2O3
3.850 SiO2
0.426 ZrO2
2268 Kasiumborat fritte (950- 1050c) [Calciumborate frit]
1.000 CaO
0.097 Al2O3
1.500 B2O3
0.609 SiO2
2279 Fritte [???? frit]
0.190 Li2O
0.350 CaO
0.187 ZnO
0.272 MgO
0.430 Al2O3
1.380 B2O3
5.720 SiO2
| |
|