Jami Jacobson on sat 10 jan 04
Does anyone have the recipe for Ferguson Gold, or Ferguson Yellow?
Thank you,
Jami =20
Yreka, CA
Gary Ferguson on sun 11 jan 04
Found the following in the archives
(http://www.potters.org/subject30567.htm):
Ferguson Yellow (for cone 6 reduction)
Custer feldspar 40
EPK 19
Dolomite 13
Whiting 8
Bone ash 6
Tin oxide 4
Flint 3
Frit 3134 7
Add:
Red iron oxide 0.3
Rutile 0.3
No relation that I know of.
:)
Gary Ferguson
Raku Clay Artist
Nampa, ID 83687
Raku Gallery and Glaze Collection at: http://www.garyrferguson.com
Subscribe to Just Raku Newsletter at http://www.JustRaku.com
Just Raku Logowear at: http://www.cafepress.com/justraku
Got Raku? Wear it here: http://www.cafepress.com/gotraku
----- Original Message -----
From: "Jami Jacobson"
To:
Sent: Saturday, January 10, 2004 4:25 PM
Subject: Ferguson Gold or Ferguson Yellow
Does anyone have the recipe for Ferguson Gold, or Ferguson Yellow?
Thank you,
Jami
Yreka, CA
____________________________________________________________________________
__
Send postings to clayart@lsv.ceramics.org
You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/
Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.
| |
|