glaze for jan 11

updated mon 12 jan 04

 

Hal Mc Whinnie on sun 11 jan 04


ARTIGAS GLAZE 675
CONE 8-10
BLUE GLOSS
custer spar 62
whiting 24
epk 17
silica 16
cobalt 1.5
rutils 15

Ron Roy on sun 11 jan 04


This glaze may not be stable at cone 8 - depends if it is melted well
enough - probably OK at cone 10 - but it will craze on most bodies.

Cobalt oxide or carbonate?

RR


>ARTIGAS GLAZE 675
>CONE 8-10
>BLUE GLOSS
>custer spar 62
>whiting 24
>epk 17
>silica 16
>cobalt 1.5
>rutils 15


Ron Roy