matt black cone 10r glaze needed

updated fri 16 jan 04

 

RubiaM&M on wed 14 jan 04


hi
my recipe
black cone 10 in redution
potash feldspar 40%
whiting 15%
epk kaolin 13%
silica 27%
add
5% cobalt oxide
5% manganese dioxide
5% red iron oxide
best regards
rubia moraes - brazil
Mr. and Mrs. Overall wrote:

>another potter in our class is looking for a matt black high fire glaze THAT "gets along with" shinos. I like the SJ Black recipe as it looks good and fit properly when overlapping, but she wants something with more texture and no gloss; not even a satin finish. Stoneware looking like. She is coupling the decoration with shinos so compatibility is a definite issue as shinos are quite selective in who they intermingle with. I've learned the hard way before reading Mel's CM article from the archives. What if a matt shino recipe had oxides added to make a black?
>
>Kim Overall
>Overall Studio
>Houston, TX
>
>______________________________________________________________________________
>Send postings to clayart@lsv.ceramics.org
>
>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/
>
>Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.
>
>Esta mensagem foi verificada pelo E-mail Protegido Terra.
>Scan engine: VirusScan / Atualizado em 07/01/2004 / Versão: 1.4.1
>Proteja o seu e-mail Terra: http://www.emailprotegido.terra.com.br/
>
>E-mail classificado pelo Identificador de Spam Inteligente Terra.
>Para alterar a categoria classificada, visite
>http://beta.terra.com.br/centralunificada/emailprotegido/imail/imail.cgi?+_u=rubiamm&_l=1074095371.325382.2808.tucuman.terra.com.br
>
>
>
>

--

http://fotos.terra.com.br/album.cgi/475962


Mr. and Mrs. Overall on wed 14 jan 04


another potter in our class is looking for a matt black high fire glaze THAT "gets along with" shinos. I like the SJ Black recipe as it looks good and fit properly when overlapping, but she wants something with more texture and no gloss; not even a satin finish. Stoneware looking like. She is coupling the decoration with shinos so compatibility is a definite issue as shinos are quite selective in who they intermingle with. I've learned the hard way before reading Mel's CM article from the archives. What if a matt shino recipe had oxides added to make a black?

Kim Overall
Overall Studio
Houston, TX