search  current discussion  categories  glazes - faults 

crawling glazes

updated fri 20 feb 04

 

Lois Ruben Aronow on mon 16 feb 04


> Hello My crawled friends.
> I add here a letter I got this morning from Trine, she is a
> Danish potter. Trine asked me about a year ago about crawling
> glazes and promised to write again, when she would finish her project.
> Her site is beautiful as a site and because of the wares she
> has made.
> Please visit her and see: You can start crawl at ^08!

I'd love to see her work. Please post her web site address.....

Diane Palmquist on tue 17 feb 04


Wonderful pots! Wish the site was in English!
Diane
----- Original Message -----
From: "Ababi Sharon"
To:
Sent: Monday, February 16, 2004 10:22 PM
Subject: Re: crawling glazes


It was in her letter (or had to be) here I resend it:
===================
Dear Ababi
I wrote you along time ago from Denmark about a project in raku and
crawling glazes, you got me started with my project, Thank you.
I have made my own website www.keramikken.dk
There you can see some of my work, see under, skøre kugler.
Have a nice day
Trine from Denmark
===================================


Ababi Sharon
Glaze addict
Kibbutz Shoval Israel
ababisha@shoval.org.il
http://ababi.active.co.il
http://www.matrix2000.co.nz/Matrix%20Demo/Ababi.htm
To Ceramics forum in Hebrew:
http://www.botzpottery.co.il/kishurim.html

-----Original Message-----
From: Clayart [mailto:CLAYART@LSV.CERAMICS.ORG] On Behalf Of Lois Ruben
Aronow
Sent: Monday, February 16, 2004 4:47 PM
To: CLAYART@LSV.CERAMICS.ORG
Subject: Re: crawling glazes

> Hello My crawled friends.
> I add here a letter I got this morning from Trine, she is a
> Danish potter. Trine asked me about a year ago about crawling
> glazes and promised to write again, when she would finish her project.
> Her site is beautiful as a site and because of the wares she
> has made.
> Please visit her and see: You can start crawl at ^08!

I'd love to see her work. Please post her web site address.....

________________________________________________________________________
______
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.

____________________________________________________________________________
__
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.

Ababi Sharon on tue 17 feb 04


It was in her letter (or had to be) here I resend it:
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D
Dear Ababi
I wrote you along time ago from Denmark about a project in raku and
crawling glazes, you got me started with my project, Thank you.
I have made my own website www.keramikken.dk
There you can see some of my work, see under, sk=F8re kugler.
Have a nice day
Trine from Denmark
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D

=20
Ababi Sharon
Glaze addict
Kibbutz Shoval Israel
ababisha@shoval.org.il
http://ababi.active.co.il
http://www.matrix2000.co.nz/Matrix%20Demo/Ababi.htm
To Ceramics forum in Hebrew:
http://www.botzpottery.co.il/kishurim.html=20

-----Original Message-----
From: Clayart [mailto:CLAYART@LSV.CERAMICS.ORG] On Behalf Of Lois Ruben
Aronow
Sent: Monday, February 16, 2004 4:47 PM
To: CLAYART@LSV.CERAMICS.ORG
Subject: Re: crawling glazes

> Hello My crawled friends.
> I add here a letter I got this morning from Trine, she is a
> Danish potter. Trine asked me about a year ago about crawling
> glazes and promised to write again, when she would finish her project.
> Her site is beautiful as a site and because of the wares she
> has made.
> Please visit her and see: You can start crawl at ^08!

I'd love to see her work. Please post her web site address.....

________________________________________________________________________
______
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.

Holly Mattox Miller on wed 18 feb 04


Diane - try http://www.tranexp.com:2000/InterTran to translate from =20
danish to english. I didn't get a full clear translation, but it was =20
enough to get a feel for what the artist was trying to say. HTH - Holly =20=

(from CLAYART)
On Tuesday, February 17, 2004, at 04:15 PM, Diane Palmquist wrote:

> Wonderful pots! Wish the site was in English!
> Diane
> ----- Original Message -----
> From: "Ababi Sharon"
> To:
> Sent: Monday, February 16, 2004 10:22 PM
> Subject: Re: crawling glazes
>
>
> It was in her letter (or had to be) here I resend it:
> =3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D
> Dear Ababi
> I wrote you along time ago from Denmark about a project in raku and
> crawling glazes, you got me started with my project, Thank you.
> I have made my own website www.keramikken.dk
> There you can see some of my work, see under, sk=F8re kugler.
> Have a nice day
> Trine from Denmark
> =3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D
>
>
> Ababi Sharon
> Glaze addict
> Kibbutz Shoval Israel
> ababisha@shoval.org.il
> http://ababi.active.co.il
> http://www.matrix2000.co.nz/Matrix%20Demo/Ababi.htm
> To Ceramics forum in Hebrew:
> http://www.botzpottery.co.il/kishurim.html
>
> -----Original Message-----
> From: Clayart [mailto:CLAYART@LSV.CERAMICS.ORG] On Behalf Of Lois =
Ruben
> Aronow
> Sent: Monday, February 16, 2004 4:47 PM
> To: CLAYART@LSV.CERAMICS.ORG
> Subject: Re: crawling glazes
>
>> Hello My crawled friends.
>> I add here a letter I got this morning from Trine, she is a
>> Danish potter. Trine asked me about a year ago about crawling
>> glazes and promised to write again, when she would finish her =
project.
>> Her site is beautiful as a site and because of the wares she
>> has made.
>> Please visit her and see: You can start crawl at ^08!
>
> I'd love to see her work. Please post her web site address.....
>
> =
_______________________________________________________________________=20=

> _
> ______
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
> melpots@pclink.com.
>
> =
_______________________________________________________________________=20=

> _____
> __
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
> melpots@pclink.com.
>
> =
_______________________________________________________________________=20=

> _______
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at =20
> melpots@pclink.com.
>
>
Yours in Christ,

Holly Mattox Miller
Reply to: millermh@hotmail.com

Ababi on thu 19 feb 04


By the way the pots are in English!
She sings My bonny is over the ocean when she makes them ( Perhaps
Scottish...)
----- Original Message -----
From: "Holly Mattox Miller"
To:
Sent: Wednesday, February 18, 2004 6:26 PM
Subject: Re: crawling glazes


Diane - try http://www.tranexp.com:2000/InterTran to translate from
danish to english. I didn't get a full clear translation, but it was
enough to get a feel for what the artist was trying to say. HTH - Holly
(from CLAYART)
On Tuesday, February 17, 2004, at 04:15 PM, Diane Palmquist wrote:

> Wonderful pots! Wish the site was in English!
> Diane
> ----- Original Message -----
> From: "Ababi Sharon"
> To:
> Sent: Monday, February 16, 2004 10:22 PM
> Subject: Re: crawling glazes
>
>
> It was in her letter (or had to be) here I resend it:
> =3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D
> Dear Ababi
> I wrote you along time ago from Denmark about a project in raku and
> crawling glazes, you got me started with my project, Thank you.
> I have made my own website www.keramikken.dk
> There you can see some of my work, see under, sk=F8re kugler.
> Have a nice day
> Trine from Denmark
> =3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D
>
>
> Ababi Sharon
> Glaze addict
> Kibbutz Shoval Israel
> ababisha@shoval.org.il
> http://ababi.active.co.il
> http://www.matrix2000.co.nz/Matrix%20Demo/Ababi.htm
> To Ceramics forum in Hebrew:
> http://www.botzpottery.co.il/kishurim.html
>
> -----Original Message-----
> From: Clayart [mailto:CLAYART@LSV.CERAMICS.ORG] On Behalf Of Lois Ruben
> Aronow
> Sent: Monday, February 16, 2004 4:47 PM
> To: CLAYART@LSV.CERAMICS.ORG
> Subject: Re: crawling glazes
>
>> Hello My crawled friends.
>> I add here a letter I got this morning from Trine, she is a
>> Danish potter. Trine asked me about a year ago about crawling
>> glazes and promised to write again, when she would finish her project.
>> Her site is beautiful as a site and because of the wares she
>> has made.
>> Please visit her and see: You can start crawl at ^08!
>
> I'd love to see her work. Please post her web site address.....
>
> _______________________________________________________________________
> _
> ______
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
> melpots@pclink.com.
>
> _______________________________________________________________________
> _____
> __
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
> melpots@pclink.com.
>
> _______________________________________________________________________
> _______
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
> melpots@pclink.com.
>
>
Yours in Christ,

Holly Mattox Miller
Reply to: millermh@hotmail.com

_________________________________________________________________________=
___
__
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.