search  current discussion  categories  glazes - cone 04-06 

need a cone 04 clear glaze

updated wed 16 jun 04

 

Trish Messenger on tue 15 jun 04


Hello everyone,
I have been having a very frustrating time the last
month or so developing a clear cone 04 glaze for my
red and white earthenware clay. I have so much bisque
that needs glazing I no longer have any shelf space.
Does anyone have a 04 base glaze that is food safe
that they would be willing to share with me?
Thank you,
Tricia



__________________________________
Do you Yahoo!?
New and Improved Yahoo! Mail - Send 10MB messages!
http://promotions.yahoo.com/new_mail

Darnie Sizemore on tue 15 jun 04


Tricia,


This is one that I use, however it is a finikie glaze, when allpied to thick it is cloudy and to thin it is chalkie. Other than that it works well.



Darnie
Cone 04 Glaze


M-1 Clear

100

500

1000

5000

7500

10,000

Nephline

Synite

17

85

170

850

1275

1700

Gillespie Borate

26

130

260

1300

1950

2600

Frit 3195

26

130

260

1300

1950

2600

Cornwall Stone

13

65

130

650

975

1300

Flint

9

45

90

450

675

900

EPK

9

45

90

450

675

900















Bentonite

(super additive)

+3

15

30

150

225

300


Trish Messenger wrote:Hello everyone,
I have been having a very frustrating time the last
month or so developing a clear cone 04 glaze for my
red and white earthenware clay. I have so much bisque
that needs glazing I no longer have any shelf space.
Does anyone have a 04 base glaze that is food safe
that they would be willing to share with me?
Thank you,
Tricia



__________________________________
Do you Yahoo!?
New and Improved Yahoo! Mail - Send 10MB messages!
http://promotions.yahoo.com/new_mail

______________________________________________________________________________
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.



---------------------------------
Do you Yahoo!?
Yahoo! Mail - You care about security. So do we.