Ross and Rox on thu 23 sep 04


I think it was Ababi Sharon who once said that this is a good engobe.

Can I try it at Cone 9 oxidation to use with Mason stains or should I
look for another engobe?

Conard's engobe for green or bisque04-8
=========================================
BORAX............... 5.00
NR POTASH FELDSPAR. 15.00
WHITING............. 5.00
ENGLISH KAOLIN...... 20.00
NEPHELINE SYENITE... 10.00
BALL CLAY........... 20.00
QUARTZ.............. 25.00
========
100.00

Thanks for any opinions. I am really trying to find ways to use mason
stains on porcelain and would like any help, book titles, glazes, etc.
Can I get it to spray? In a small sprayer? Or will it clog?

I am so totally inexperience with Mason stains, but ready to learn!

Roxanne in OR where it was 83 degrees and sunny!

Ron Roy on sat 25 sep 04


Hi Roxanne,

I just compared this to a cone 6 porcelain and it's going to melt a lot
lower - maybe it's for low fire ware.

Best to do some serious testing before slapping it all over you work.

RR


>Can I try it at Cone 9 oxidation to use with Mason stains or should I
>look for another engobe?
>
>Conard's engobe for green or bisque04-8
>=========================================
>BORAX............... 5.00
>NR POTASH FELDSPAR. 15.00
>WHITING............. 5.00
>ENGLISH KAOLIN...... 20.00
>NEPHELINE SYENITE... 10.00
>BALL CLAY........... 20.00
>QUARTZ.............. 25.00
>========
>100.00

Ron Roy
RR#4
15084 Little Lake Road
Brighton, Ontario
Canada
K0K 1H0
Phone: 613-475-9544
Fax: 613-475-3513