take some loose kaowool blanket, fiberfax etc.
mix it with itc 100, or some troweleze. be creative.

fill the crack. fire the kiln.
fixed.
even overhead. and, the crack does not push out the
material.
fixed as good as new.

it is the slight flex of the kaowool that makes the
crack get fixed right.

if you fill a crack with a clay based mortar, the crack
gets bigger, and pushes the mortar out.
now the crack is really big.

isn't that jean lutz just a smarty pants girl.
makes her own numbers, any size on the computer.
then makes a stencil. makes house numbers, and can
sell them for at least $4.63. rich i tell you, rich.
god, the world is getting better.

and, tom sawyer....out of whine, wine....
and we send a hug.
even if he is agnostical medical doctor,lawyer, potter and
flower grower.
damn god, damn hurricane, damn sun.
damn rain.
but, it does no good.
nature is here to stay.
mel
i think dan rather caused this hurricane.
From:
Minnetonka, Minnesota, U.S.A.
web site: my.pclink.com/~melpots
or try: http://www.pclink.com/melpots
new/ http://www.rid-a-tick.com