Glaze test for Emmanuel Cooper Speckled Transparent, cone 5-6.

Glaze tested on white midrange stoneware fired in electric oxidation to =
1240c. (2264f)

Source: Clay Times Nov/Dec. 2004
Credited to: Emmanuel Cooper

Firing ramp:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)=20
80c p/h to 1240c (176f - 2264f)
5 min. soak
cool down max. to 800c (1472f)
Hold 1 hour
Shut off kiln

Recipe:
25 Nepheline Syenite
35 Frit 3134
20 China Clay
20 Silica

ADD
7 Rutile

Note: All raw materials are measured up or down to the nearest whole =
decimal. =20
Colorants or additives to a 100 gram test batch are measured in percent =
to the 100 gram test batch.

Results:
Clear gloss, claybody has an overall toasty color under glaze.

Regards from Alisa in Denmark