> it is the farthest right column on the porcelain page.

Jessy, here is the recipe on the farthest right on Page 34 of Cushing's
Handbook. It's called Jeff Cole Porcelain - translucent.

55 Grolleg
35 Kona F-4 Feldspar
15 Flint
3 Macaloid

The following information is also included:

Fire to cone 9 down and cone 10 soft. This body will slump if fired to
cone 10 down. Very translucent.
When making this body, add 3% Macaloid to 30 lbs. of water. Let it sit
overnight. Then add to 100 lbs dry clay.

Regards,