Mim, here's a nice opaque copper pink:

G449 Cone 10 Reduction

Custer spar - 3550 gm
Silica - 3550 gm
Whiting - 1540 gm
Gerstley borate - 1010 gm
EP Kaolin - 150 gm
Tin oxide - 150 gm
Copper carbonate - 50 gm

Good luck!