This is what we use here. Works great on Brown or White clay.

Gerstley Borate

Gary Lee on thu 2 jun 05

=?ISO-8859-1?Q?=20glaze?=

Well, I try again.............. This is the white we use here and it works
great at cone 5 or 6.



Gerstley Borate 840

Wollastonite 320

Neph Syenite 1200

EPK 400

Silica 1240
____________
4000 grams

Ziropax 400 this is 10% of the above 4000 grams.

You can vary the whiteness by increasing or decreasing the % of ziropax.