search  current discussion  categories  kilns & firing - shelves & furniture 

low fire clay body recipe

updated tue 24 jan 06

 

annapoorna sitaram on sun 22 jan 06


hello
we are trying out various low fired (temp 1050 -1060 C) I have yet to
find a very nice plastic body without talc.Are there any,I been on the
net and have not found any low fire without talc bodies.
thanking you in advance
annapoorna

John Britt on sun 22 jan 06


Annapoorna,

Are you interested in white or iron bodies?

John Britt
www.johnbrittpottery.ocm

John Britt on mon 23 jan 06


Annapoorna,



There are a lot to choose from. But here are two to get you going:





VC EARTHENWARE RED

Cone 05

10.00 Grolleg Kaolin

15.00 Kentucky Ball Clay

15.00 Goldart

35.00 Ocmulgee Clay (Lizella)

15.00 F-4 Feldspar

10.00 Ferro 3134

1.00 Veegum T (Macaloid or Bentonite)



WHITE VITREOUS Body Cone 05

12.00 Tile #6 Clay

20.00 EPK Kaolin

26.00 C and C Ball Clay

10.00 Nepheline Syenite.

28.00 Ferro 3124

2.00 Gerstley Borate

2.00 Bentonite




Hope it helps get you started,



John Britt
jPresident of the Glazes Free Trade Society
www.johnbrittpottery.com