Here's my slip/glaze contribution. As with all glazes
and slips it all takes physical testing to get there
from here. The comments section will help reduce that
time. The clay content is 50% with dolomite inclusion
and 3124 to flux the materials. High AL203 low SiO2
with a low mid B203 level. Recommeded for exterior
decorative pieces when used as a thinned down glaze or
as a slip when used as a paste or thickened.

Edwards Matte Slip Glaze (C)
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone ^ 6 Ox
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

OM-4 Ball Clay 40.00
Ferro 3124 30.00
Dolomite 20.00
EPK Kaolin 10.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.117 3.14%
CaO 0.597 13.26%
MgO 0.285 4.55%
Al2O3 0.525 21.16%
B2O3 0.180 4.95%
SiO2 2.201 52.33%
TiO2 0.020 0.62%
K2O 0.021 0.78%
Na2O 0.096 2.36%
Al:Si 4.19
Expan. 9.39
ST 358.06
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Opacity-Opaque
Texture-Clean Matte
Stability-Stable
Fit-(Test on various clay bodies)
Last changed: 03/03/02
Status-tested
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,


Bill Edwards
http://apottersmark.blogspot.com/

'Studio Pottery Set-up for Sell, offers considered!'

__________________________________________________
Do You Yahoo!?
Tired of spam? Yahoo! Mail has the best spam protection around
http://mail.yahoo.com