Cone 6 Variation

kevin finegan on thu 4 may 06


I thought I'd posted this last night but it hasn't shown up yet, so I'll try again
Karen Starshine ^6 from Val Cushing's Glaze Book

K-200 Feldspar 46.00
Soda Ash 5.00
Gerstley Borate 12.00
Whiting 10.00
Barium Carbonate 5.00
Lithium Carbontate 2.00
Flint 20.00
Add:
Macaloid 2.00
Titanium 4.00
Copper Carbonate 5.00

I haven't tested this glaze for safety, so I wouldn't recommend it be used for food surfaces. I' ve used it in oxidation, though the recipe states it can be used in both reduction or oxidation. Enjoy!
Kevin in San Antonio


Crista Nelson wrote: In a message dated 5/3/2006 4:17:57 P.M. Central Daylight Time,
kevinfinegan2003@YAHOO.COM writes:

Cone 6 Variation

______________________________________________________________________________
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.



---------------------------------
New Yahoo! Messenger with Voice. Call regular phones from your PC and save big.